Procedure: Resin drying and handling (b-drying-handling). Revision 6 — October 18, 2026. Hopper sizing, regrind and desiccant added from Mike's notes. Index: https://ancreationoffice.com/sop.txt Source: Mike's practice (Mike's notes, kept private). Lines marked "Mike" are his practice; "published" lines cite the library; anything else the office adds is marked "office". Tier: deep. Read this when a resin must be dried (nylon, PC, PET, PBT, ABS and other engineered resins), a process drifts or the parts show splay, the nozzle spits, a dryer "isn't keeping up", a plant adds dryers, or regrind goes into a process. Calculations: https://github.com/mminwi/an-creation-office/blob/main/specialists/calcs/drying.py (hoppers and dryers), https://github.com/mminwi/an-creation-office/blob/main/specialists/calcs/regrind.py (regrind generations). WHY IT MATTERS Wet resin makes the process wander (Mike). Water turns to vapor in the barrel: the melt flows easier than it should, the parts show splay, and the nozzle spits and sputters as the gas escapes. Published: nylon must be molded dry; moisture degrades the polymer and costs surface quality and strength (BASF Ultramid brochure, library: resin-design-guides). 1. TEST THE DRYER; DON'T TRUST ITS METER (Mike) - The most common problem: plants run dryers nobody has ever tested. A dryer with dead desiccant is only a hot air dryer. Warm air preheats the pellets and helps a lot, but not enough for nylon and many engineered resins. - Buy a dew point tester and measure the air going into the hopper yourself. - Don't believe the dryer's own dew point display. If it reads -40 seconds after start-up, it is only telling you the machine is on. - How a twin-bed desiccant dryer starts: it regenerates (cooks) one bed first, and switches to it after roughly 30 minutes to an hour. Until then it is only heating. Test after the first bed has been regenerated and switched in, not before. 2. TEST THE RESIN (Mike) - Use a moisture analyzer: it heats a resin sample and reports percent water. There is no substitute if you run resin that needs drying. - Compare the reading with the resin maker's moisture limit for molding. 3. CHECK THE PLANT'S POWER: REVERSE PHASE KILLS DRYERS (Mike) - Some three-phase outlets get wired with the phases reversed. A dryer plugged into one runs its fans backwards: the air goes over the desiccant without passing the filter first. Resin dust coats the desiccant, the regeneration heat melts it on, and that desiccant is finished; no amount of regenerating brings it back. - Dryers get wheeled around and plugged in wherever, and desiccant is often replaced only every five years or so. One or two bad outlets can quietly ruin every dryer in the building. A new dryer plugged into the same outlet goes bad too, so replacing dryers does not fix it. - Test every outlet with a plug-in phase rotation tester: phase rotation and ground, on 220 V and 440 V three-phase. Check that dryer fans and blowers turn the right way. - Replace desiccant every year whether it seems to need it or not (Mike's practice with mostly engineered resins). Keep the replacement date on each dryer. - Office: fixing wiring is a job for a qualified electrician; testing live outlets follows the plant's electrical safety practice (NFPA 70E in the library). 4. GRINDERS AND REGRIND (Mike) - Reverse phase runs grinders backwards too. A backwards blade pulverizes the regrind into dust; the dust gets conveyed into the dryer and seals the desiccant the same way. - Be careful with regrind generally: it brings fines and dust. - Regrind levels and color: section 7. 5. THEN DRY TO THE RESIN MAKER'S NUMBERS (Mike) - Drying temperature, time and dew point: do exactly what the resin maker says. If it says four hours at a given temperature, that is what it is. With good dryers, good drying hoppers and good hoses, nine times out of ten that is all it takes. - Dryer and hopper come as a pair: the dryer or hopper maker will size the dryer for you. 6. SIZE THE HOPPER TO THE PRESS (Mike: the more critical part) - The resin must stay in the hopper at least as long as its drying time. Hopper capacity = drying time x pounds per hour through the press. Four hours at 100 lb/hr needs a 400 lb hopper; a 30 lb hopper on a 100 lb/hr press empties every 20 minutes and never dries anything. Never less than about an hour in any case. - Old hoppers that feed down the center (funnel flow) need about 1.5 to 2 times that: in a 600 lb old hopper often only 300 to 350 lb actually moves; the rest sits on the walls and never cycles. Mike's example: 4 hours at 100 lb/hr is 400 lb in a good hopper, about 600 lb in an old one. - Newer hoppers flow down more evenly (all of it moves), so they can be sized at drying time x throughput. - The proof is the resin: pull a sample at the throat, test it on the moisture analyzer. That is how you find a hopper that only flows down the center. - Published: the same rule, hopper capacity = drying time x throughput (Conair drying manuals, library: oem-dryer-guides). The calculation does this, with the old-hopper factor. 7. REGRIND (Mike) Levels: - Injection molding: about 25% is the normal limit, and the near-universal rule; test the parts at 25%. On engineered resins especially, don't go over 25%. Plants sometimes creep up toward 50% to use regrind up; that is a choice to make knowingly, not the standard. - Blow molding: 50% regrind is common, because the process makes so much trim and flash. - White, very light colors and clear: zero regrind. It goes from 25% straight to zero; the visual defects aren't worth it. - The standard regrind note on most customers' drawings is 25% (Mike). Whatever the drawing or spec says wins. Generations: what you are really running (Mike: "a great one for AI"): - At steady state, part of the regrind has been through the press two, three, four times. At high regrind the old generations become a big share. Run the table (regrind.py) for the percentage you plan: - 25%: virgin 75%; material 3 or more generations old is about 1.6% of the feed. - 50%: virgin 50%; 3 or more generations old is 12.5% of the feed (a quarter of the regrind). - 60%: virgin 40%; 3 or more generations old is about 21.6% of the feed (over a third of the regrind). - Physics of the table: with regrind fraction r fed back continuously, the share that has been through k times before is (1 - r) x r^k; the average pellet has r / (1 - r) earlier heat histories. First ask what the color is for (Mike): - Coding color: the color tells people what the part is ("red means this size"), or the part is black for UV resistance or just to be black. Mixing regrind across colors, as below, is fine within limits. - Matched color: the part has to match something, such as a car's interior red, or it is a critical appearance part. Then don't mix other colors' regrind into it at all, whatever the color, black included. Where the light-colored regrind goes (coding colors only): - Don't put white regrind back into white. Run it into gray or another color, but only a little: white lightens other colors fast. - Black (made for UV resistance or plain black, not matched) is the best place for it: black covers. Black colorant is usually loaded about three times heavier than needed for color, because it is also there to stop UV degradation (block sunlight within the first few thousandths of a wall), so it hides almost any other color mixed in (Mike). WHAT THE AUDIT PRODUCES A drying audit in its own dated folder: - Per hopper: capacity, old (center flow) or new (even flow), throughput through it, drying time, and resin moisture at the throat. - Per dryer: tag, desiccant age, outlet it uses (phase rotation and ground: pass/fail), fan and blower direction, filter condition, the dryer's displayed dew point, the measured dew point after a full regeneration and switch-over, and the hopper size against throughput and drying time. - Per resin: the maker's drying temperature, time, dew point and moisture limit; measured moisture at the press. - Per grinder: rotation direction, fines in the regrind; regrind percentage in use against 25% (and any customer limit). - Findings in order: wrong-phase outlets (fix first, before any dryer is replaced), dead desiccant or desiccant older than a year, undersized or center-flowing hoppers, resin above its moisture limit, regrind fines. Recommendations are proposals; Mike or the plant confirms. HANDS OFF Electrician for outlet wiring; the dryer maker or service company for desiccant replacement; the resin maker for drying conditions. OPEN FOR MIKE - How often to re-test dryers with the dew point tester (the office proposes: at start-up of every new dryer, after desiccant replacement, and whenever parts show splay).